Abstract
Tablet dimensional changes are one hurdle in continuous coating. The aim of the present study was to evaluate whether a time period of tablet core relaxation is needed prior to coating. The conditions for the experiments were chosen such that maximum tablet core dimensional changes were achieved as challenge for subsequent coating. Three powder blend compositions containing the (super)disintegrants Starch 1500® and/or crospovidone resulting in tablet cores with different relaxation tendency were coated immediately or 24 h after compaction with three immediate release Opadry® coatings of variable flexibility to show a potential impact on the coating quality.
‘Dry’ and ‘moist’ coating conditions were applied by variation of the coating suspension spray rates. The tablets increased significantly in tablet dimensions depending on their formulation. Despite these dimensional changes, the quality of the coatings was satisfactory as no defects were found. In addition, no differences were observed in the coating thickness of the three coated tablet formulations. The expected defects in the coatings were only found under high humidity storage conditions. In conclusion, the presented results revealed that no relaxation time interval between compaction and coating was necessary, indicating only minor relevance of the elastic relaxation in (continuous) tablet coating following continuous direct compression.
Introduction
In recent years, there has been a shift in pharmaceutical manufacturing towards continuous direct compression (CDC) of tablets because of the inherent economic benefits compared to traditional supply chainsCitation1. A fully CDC line includes feeding, powder blending, and tablet compaction, while the addition of tablet coating and subsequent direct packaging makes the impact on the overall Oral Solid Dosage form (OSD) production even more significant. Although intensive research has been performed on several steps of continuous production lines, the link between the compaction and coating processes has not yet been fully investigated. Especially, the storage interval between these two processes which is supposed to be necessary for tablet elastic relaxation, needs to be questioned.
The driving force of tablet elastic relaxation has been suggested to be the elastic energy stored in the powder bed during densificationCitation2, Citation3. The elastic relaxation itself is understood as the release of that portion of internally stored energy which is not used for the formation of tight particle bonds during compactionCitation4. Instead, it leads to an expansion of the tablets resulting in an increase of tablet dimensions depending on factors such as the physicochemical properties of the ingredientsCitation3. Elastic relaxation may be distinguished in a fast in-die and a slow out-of-die elastic relaxation. Fast in-die elastic relaxation is defined as the change of the tablet dimensions within the time period between maximum compression and tablet ejection.
Slow out-of-die elastic relaxation refers to tablet dimensional changes during storage and of viscoelastic nature. It has been shown, that the storage conditions, especially temperature and humidity, affect tablet dimensional changes to a great extentCitation5. Various methods for the determination of elastic relaxation such as laser triangulationCitation6, automated measurement with a micrometer screwCitation7, and transducer displacementCitation8 have been described in the literature. However, the feasibility of these methods for the investigation of tablet dimensional changes under simulated storage conditions is limited. Several studies based on these methods reported a pronounced tablet elastic relaxation under the following tableting parameters: low turret speeds (long dwell times)Citation9, Citation10, high compaction forcesCitation11, high tablet diametersCitation12, and the selection of powder blends with a high relaxation tendencyCitation8.
In continuous manufacturing this expansion of the tablets might impair the (continuous) coating process because of the possible formation of cracks in the coating filmsCitation5, Citation13. The hypothesis of internal stress in coating films which cannot be compensated for by the mechanical properties of the coating material is still being discussedCitation5, Citation14. Coating defects such as cracking, splitting or bridging might occur if the internal stress within the coating film exceeds its mechanical properties such as the tensile strength and the elastic modulus of the polymer. These defects are likely to be found in the side regions of the coated tablet, as the dimensional changes of the tablet cores after compaction occur primarily in the axial direction as a result of the uniaxial compaction process. Indeed, it was shown that the coating thicknesses in these regions are particularly thinCitation15. Defects in the coatings are inevitably linked to a loss of function and might have consequences regarding OSD stability and drug releaseCitation13.
In many production facilities, continuous tablet coating is avoided for these reasons or technical solutions such as intermediate storageCitation16 or heated and extended tablet dedusters are used to prolong the time interval between tablet ejection and transfer to the coater. In batch manufacturing of coated tablets, it is common practice to store the tablet cores for at least 24 h prior to coating to prevent potential coating defects resulting from tablet relaxationCitation9.
To date only one published study exists, in which the feasibility of an in-line coating process for starch-based tablet cores using a flexible coating polymer is demonstratedCitation6. Further studies are needed with coating polymers differing in their mechanical properties to identify polymers which withstand potential dimensional changes during and after compaction. Efficient continuous coating is associated with short process times and high spray ratesCitation17. However, the influence of the spray rate has not yet been thoroughly investigated with regard to tablet dimensional changes and the stability of the coatings.
A systematic comparison of the coating efficiency of tablet cores with different extents of relaxation, directly after compaction and after an appropriate time of relaxation, is necessary to assess the relevance of tablet elastic relaxation in continuous coating. For those reasons, the aim of the present study was to focus on the need for a time interval between compaction and coating of tablet cores to allow for relaxationCitation9 under relaxation-promoting conditions. Furthermore, a new telemetric method to optically measure tablet dimensional changes under defined conditions was introduced.
Download the full article as PDF here Challenging the paradigm of tablet relaxation in continuous coating
or continue reading here
Materials
Table 1: Powders used for tablet preparation
| Material | Brand/Grade | Supplier |
|---|---|---|
| Microcrystalline cellulose (MCC) | Avicel® PH 101 | FMC (Philadelphia, USA) |
| Pregelatinized maize starch (PGS) | Starch 1500® | Colorcon (Indianapolis, USA) |
| Agglomerated lactose (LAC) | Tablettose® 80 | Meggle (Wasserburg am Inn, Germany) |
| Crospovidone (PVPP) | Kollidon® CL | BASF (Ludwigshafen, Germany) |
| Magnesium stearate (MgSt) | Ligamed MF-2-V MB | Peter Greven (Bad Münstereifel, Germany) |
Lutz, D., Bekaert, B., Crönlein, J., Grymonpré, W., & Leopold, C. S. (2026). Challenging the paradigm of tablet relaxation in continuous coating: analysis of tablet dimensional changes after continuous direct compression. Pharmaceutical Development and Technology, 1–26. https://doi.org/10.1080/10837450.2026.2761632